GATE 2023 XE — all source sections – Question 130
A continuous and aligned glass-fiber reinforced composite consists of 40 vol% of glass-fiber having a modulus of elasticity of 69 GPa and 60 vol% of a polyester resin, which when hardened, displays a modulus of 3.4 GPa. The modulus of elasticity of this composite in the longitudinal direction is___________GPa. (Rounded off to two decimal places)
Practise this question in The GATE Grind →
Show answer and explanation
Correct answer: 29.60 to 30.01
Explanation
Aligned continuous fibres under longitudinal isostrain give Ec = VfEf + VmEm. Thus Ec = 0.4 × 69 + 0.6 × 3.4 = 29.64 GPa. The volume fractions already sum to one, and no density-based conversion is needed. This is distinct from the transverse inverse-mixture approximation.